9.1 Introduction
During the construction of asphalt pavements, two types of joints are encountered. The first is a transverse joint, which is constructed whenever the paving operation is interrupted for a period—anywhere from 15 min to several weeks or more. The second is a longitudinal joint (LJ), built when a lane is constructed adjacent to a previously placed lane of mix (see Figure 123). Both types of joints are key to performance; transverse joints have a significant impact on smoothness, while LJs greatly impact long-term durability.
Transverse joints have a significant impact on smoothness, while longitudinal joints (LJs) greatly impact long-term durability.

Source: National Asphalt Pavement Association
Figure 123. Longitudinal Joints on Airfield Runway
Joint deterioration starts when air, water, and contaminants find their way into the joint, through either segregation, poor density, or the two mats not bonding properly. Because the linear distance of LJs is so much greater than the linear distance of transverse joints, both on roadways and airfields, discussion around joint durability and joint deterioration is generally focused on the LJs.
Typical distresses near the LJ are cracking and raveling (see Figure 124). As the joint deteriorates, it will require additional maintenance such as joint sealing, patching, or premature resurfacing. Since there are typically numerous LJs on a pavement, their performance is vital for the overall performance of a project. Unsatisfactory LJ performance has often been the weakest link in an otherwise long-lasting asphalt pavement.

Source: Asphalt Institute
Figure 124. Premature Deterioration of Longitudinal Joints
For airfields, cracking and raveling around the LJ leads to loose material on the pavement surface and is a major source of FOD that can be ingested and damage aircraft engines, as discussed in Section 1.2.
9.1.1 Chapter Outline
The techniques for constructing each type of joint are discussed in this chapter and were intentionally omitted from the two previous chapters on Mix Placement and Compaction to consolidate the discussion of joints here.
Transverse joints, also referred to as construction joints, are covered first, followed by a lengthy section on LJs. Echelon paving, a method that reduces the number of cold LJs, has its own section. The last section mentions some new LJ treatments and methods. Airfield considerations and techniques that are more prevalent for airfield paving, such as cutting back the LJ, are integrated within the appropriate sections of this chapter.
9.1.2 Terminology
When discussing both transverse joints and LJs, the following terms need to be defined (see also Figure 125):
Cold side, or unconfined side—the first side of the joint that was placed and allowed to cool before the other side of the joint was placed. This side has had the opportunity to cool after compaction and thus is referred to as the cold side of the joint. For LJs, it is also referred to as the cold lane. Because the mat was placed and compacted without any lateral confinement under the roller, it is also referred to as the unconfined side of the joint. The lack of confinement makes densification under the roller more challenging and is why specifications for airfield pavements call for cutting back and removing several inches of this lower density material.
Hot side, or confined side—the second side of the joint that was placed. This side is placed and compacted hot, next to the cold side, and thus is referred to as the hot side of the joint. For LJs, it is also referred to as the hot lane. Because the mat is placed next to a mat that has already cooled and stiffened, the mat under the roller is confined laterally. Because of the confinement, achieving density on this side of the joint is typically easier. One of the biggest problems on the hot side of the joint is failing to ensure that sufficient thickness of material (25 percent rolldown) is placed to allow for density to be obtained as the material is rolled down even with the cold side. This topic is covered in detail in Section 9.3.3.2.
Hot joint versus cold joint—The term hot joint refers to the circumstances where two lanes of mix are placed, and both lanes remain hot enough to allow for adequate compaction on both sides of the joint. A typical temperature limit in airfield specifications to distinguish between a hot joint and a cold joint is 175 °F, meaning if the mix temperature drops below 175 °F, it must be treated as a cold joint due to difficulty in achieving adequate density. Echelon paving is a technique that creates hot joints instead of cold joints.

Source: Asphalt Institute
Figure 125. Common Terms for Transverse and Longitudinal Joints
9.2 Transverse/Construction Joints
Watch Video
9.2.1 At End of Paving Operation
When a paving operation is suspended in the middle of a project, whether overnight or for an extended period, a transverse construction joint is required.
For airfields, it is desirable for the paving at the end of the day to end at the area being paved, such as the end of a runway, to reduce the number of transverse joints, which will tend to increase smoothness and minimize FOD.
For airfields, it is desirable for the paving at the end of the day to end at the area being paved, such as the end of a runway, to reduce the number of transverse joints.
When a transverse joint is required, it is important that the paver be run in normal fashion right up to the point at which the transverse joint will be located. The head of material in front of the screed should remain constant up to the location of the joint so the forces acting on the screed are constant and a consistent angle of attack is maintained.
A good practice is to locate the transverse joint at a point where the head of material in front of the screed is normal. It is a poor practice to run the hopper out of mix before the location where a transverse joint is to be built. When this is done, the amount of mix carried on the augers is reduced, as is the head of material in front of the paver screed, causing the screed angle to fall. The thickness of the mat will then gradually decrease leading up to the joint location. This will result in a low point on the new pavement surface.
When paving resumes, an almost vertical face is needed on the cold side of the joint. Creating that vertical face, whether the joint was temporarily opened to traffic or not, is discussed in the next section.
If opened to traffic, the transverse joint needs to provide a safe, smooth transition for vehicles dropping from the level of the new surface down to the existing surface. The easiest way to do this is to build a temporary wedge of material to ramp traffic down to the underlying surface. This wedge is removed before paving operations resume.
9.2.1.1 Temporary Ramp for Traffic
There are three methods paving contractors can employ for properly building the sacrificial wedge:
- Stop the paver and lift the screed over the head of material in the auger area. Then separate the excess material by shoveling a transverse trench in the fresh mix on the downstream side of the joint. Push back the face of the joint line with a lute or rake to make a sharp vertical edge on the side of the joint that remains in place. Use a bond-breaking material (plastic or Kraft paper) to line the bottom of the wedge area and cover the vertical face (see Figure 126). After lining the area with a bond breaker, move excess mix onto the bond breaker and rake it into a wedge. The whole area is then compacted.
- In a variation of the previous method, insert a wooden block or bulkhead the same thickness and width as the compacted mat after lining the area downstream of the lateral joint with the bond breaker. This block will remain in place to provide a true vertical face on the cold side of the joint and facilitate the removal of the sacrificial wedge of material when paving resumes. Care should be taken to prevent a bulkhead from becoming dislodged if opened to traffic. Prolonged exposure to traffic may require pinning or nailing down blocks or bulkheads.
- If the temporary wedge is going to be used by traffic for only a short time (e.g., overnight), the application of the tack coat under the wedge can be eliminated, which will greatly facilitate removal. After selecting and marking the joint location, stop the tack coat application at the marked joint location. As the paver passes the joint location, shut off the material delivery conveyors, stopping the flow of material into the screed area. As the screed is starved of material, the thickness of the mat drops until the mat thickness is feathered out to zero.
Note that these methods of building a temporary wedge for traffic to be opened will typically not be used for airfields.

Source: Asphalt Institute
Figure 126. Placement of Kraft Paper Bond Breaker on Transverse Joint
9.2.1.2 Rolling Transverse Joint at End of Paving Operation
Depending on whether the transverse joint is a butt joint or has a temporary wedge for traffic, the recommended rolling operation to compact each at the suspension of paving is different. For a butt joint, a board that is the thickness of the compacted layer should be placed at the end of the transverse joint to allow the front drum of the roller to compact past the end of the mat and to protect the vertical face. For a tapered wedge joint, the front drum of the roller can roll over the transverse joint and tapered mat without significant concern for rounding off the mat edge at the top of the joint.
9.2.1.3 Removing Temporary Ramp and Creating Vertical Face
When paving resumes, the sacrificial wedge of material and, if used, the wooden block and bond breaker material are removed and disposed of properly.
The cold mat is cut back on a straight line to the point where full mat thickness exists transversely. When doing the cutback, a power saw equipped with either a dry-cut diamond or abrasive-blade is used. A water-cooled saw should never be used as it will produce a wet slurry that leaves a dust film on the vertical face. Some specifications, particularly on airfields, require all transverse joints be cut back with a dry pavement saw to ensure a true vertical face.
A cold-milling machine running transversely across the pavement may also be used to remove the wedge, if allowed per the specification. Cold milling in the longitudinal direction to remove the wedge should not be allowed as the cutting mandrel cannot create a vertical face.
After removal of the wedge, the area underneath must be cleaned and dried. Tack is applied to both the vertical face of the transverse joint and the horizontal surface of the wedge area. The tack on the vertical face will allow the hot side of the joint to adhere to the cold side and seal out moisture and contaminants that will cause the joint to ravel. When constructing a transverse joint, it is a good practice to use a 10-ft (3-m) straightedge to check the pavement leading into and away from the joint for smoothness across the joint. However, the FAA and DoD specify a 12-ft straightedge for this purpose. Doing this check while the mat is still hot allows corrections by adding or removing material to achieve acceptable mat smoothness.
9.2.2 Restart of Paving
The screed should be checked for warping and/or wear and then aligned and lowered onto wood starting blocks or lath. When starting a paving pass, blocks should be stacked to the thickness of the new mat plus an additional 25 percent allowance for rolldown. Rolldown (covered in Section 7.5) may be less than 25 percent depending on the mix. When continuing a paving pass after the construction of a header, the starting blocks are placed on the previously laid cold mat with enough thickness to match only the anticipated rolldown under compaction.
The use of these “starter blocks” holds the screed flat at its anticipated equilibrium level as it moves into fresh mix in front of the screed. This minimizes the screed’s rising or falling (introducing roughness at the joint) and significantly shortens the length of travel required for the screed to find equilibrium.
The following are steps specific to the paver that should be accomplished at startup:
- Center the tow points on both sides of the paver so they have the maximum amount of vertical adjustment to provide the necessary depth correction.
- Zero or null out the screed angle of attack by turning the depth screws to a free-rotary movement of less than 1/2 to 3/4 of a turn in both clockwise and counterclockwise directions. Check both sides to ensure that the screed is resting flat on the starting blocks. Induce the angle of attack by turning the depth screws in the appropriate direction. Previous experience with a similar mix will make setting the angle of attack easier.
- If automatic grade and slope controls are used, position the grade sensor at the correct vertical distance off the grade reference. Once the grade sensor is set, the null or neutral button on the grade controller should be pushed to finish setting the automatic grade sensor. If using the slope control system, set the angle of attack, dial in the proper slope, and use the reset button to null out the system.
- After filling the receiving hopper, monitor the mix as the drag-slat conveyor and augers fill the area in front of the screed. If material does not automatically fill the outside corners, shovel the mix to the ends to fill the screed properly. Then, check material sensors at the ends of the screed to ensure they are operating properly and set to index off the live (flowing) mass of material.
- After the paver pulls off the joint, use a straightedge and a carpenter’s level to double-check the specified slope. Also, repeatedly check the thickness with a depth probe over the first 25 ft (7.6 m). As soon as true grade and slope are established and confirmed, the controls should take over and maintain the desired profile.
9.2.3 Rolling Transverse Joints After Restart of Paving
The rolling procedure will depend on whether the LJ is confined or unconfined by the adjacent lane. When the LJ is confined by the adjacent lane, the first roller pass is made with a static steel-drum roller moving parallel to the LJ for a few feet, with the drum mostly on the cold side of the joint and overlapping the new mat by approximately 4 to 6 inches (100 to 150 mm). The surface is then checked with a straightedge and corrections made if necessary.
The transverse joint is then rolled transversely, with approximately 6 inches (150 mm) of the drum width on the newly laid material. This operation should be repeated with successive passes, each covering an additional 6 to 8 inches (150 to 200 mm) on the new mat, until the entire width of the roller is on the hot material. When the LJ is unconfined, this joint (edge) needs to be protected from the rollers. During transverse rolling, wooden boards the thickness of the compacted mat should be placed at the edge(s) of the pavement to give the roller a surface to drive onto and off the mat without causing the edge to deform (see Figure 127). The use of boards is recommended to avoid excessive shoving of the mix and to expedite the compaction process, but it may infringe on the adjacent pavement lane carrying traffic. If boards are not used, transverse rolling must stop 6 to 8 inches (150 to 200 mm) short of the outside edge to prevent damaging it, and the edge must be compacted later during longitudinal rolling.

Source: Asphalt Institute
Figure 127. Rolling the Hot Side of a Transverse Joint
Paving and compaction must be accomplished so that the completed transverse construction joint has a smooth transition across the joint and specification density has been achieved on both sides of the joint.
9.3 Longitudinal Joints
Watch Video
The outline of this section follows the same sequence of steps as when an LJ is constructed:
- Placing the Unconfined Side (Edge)
- Rolling the Unconfined Side
- Placing the Confined Side
- Rolling the Confined Side
9.3.1 Placing the Unconfined Side (Edge)
Proper construction of LJs starts with the laydown of the first lane. When the cold lane is placed, there is at least one unconfined edge of the mat. The unconfined edge must be constructed in a straight line. In the case of paving in a curve, the edge should be smooth. The use of a stringline and paint, with a guide mounted to the paver, should be employed to ensure a straight edge on the cold lane (see Figure 128). Edges that are not straight (see Figure 129) will be difficult to match with a consistent overlap (as discussed later in the chapter) when paving the hot side of the joint. This significantly increases the potential for low-density areas near the joint.
The use of a stringline and paint, with a guide mounted to the paver, should be employed to ensure a straight edge on the cold lane.

Source: Asphalt Institute
Figure 128. Paving in a Straight Line with Stringline, Skip Paint, and Guide on Paver

Source: Asphalt Institute
Figure 129. Not Paving Straight (or Smooth on a Curve) Makes It Impossible to Achieve a Consistent Overlay
9.3.1.1 Planning the Location of Longitudinal Joints
LJs should be located staggered (offset) from the underlying mat’s LJ by at least 6 inches (see Figure 130). If LJs are placed directly on top of each other, there will be a greater tendency for cracking to occur at the joint through the various lifts. Many specifications, including the DoD and FAA airfield specs, require the LJ to be offset a minimum of 1 ft from the LJ of the underlying layer.

Source: Asphalt Institute
Figure 130. Staggered Joints
When paving projects with multiple lifts, the location of LJs on all lifts should be planned with this minimum offset in mind. If the roadway or airfield feature is crowned at the center, it is desired for the location of the LJ on the surface lift to also be at the centerline. When possible, it is best to plan LJ locations so that the LJs on the surface lift do not fall within traffic wheel paths, recessed pavement markings, or striping. This is not generally possible on airfields.
There are three types of conventional cold LJs, as seen in Figure 131: butt, notched-wedge, and milled or cutback. Each will be described in the next three sections.

Source: Asphalt Institute
Figure 131. Different Types of Longitudinal Joints
9.3.1.2 Butt Joints
The butt joint is the most common type of LJ. While placing the unconfined side, butt joints start with a fairly vertical edge, assuming the end gate is set down properly by riding on the existing surface. Full screed vibration (leaving the screed vibrator on) assists mix consolidation at the bottom of the joint. After the mat is placed and during compaction (discussed in the next section), the mat’s edge tends to seek its own angle of repose (less vertical).
Figure 132 shows the poor practice of setting the end gate higher, which allows the mix to flow under the end gate, leading to very low density after compaction on the unconfined edge. Setting the end gate properly, firmly seated on the existing pavement surface, prevents this.

Source: Asphalt Institute
Figure 132. Poor Practice—End Gate Not Set to Be Seated on Existing Surface
Unsupported butt joints of substantial thickness opened to traffic may create hazardous drop-off conditions for motorists. The Manual on Uniform Traffic Control Devices (MUTCD) provides recommendations for signage to warn motorists of unexpected conditions. Where excessive drop-offs are necessary, it may be best to close the adjacent lane or use a notched-wedge joint (discussed next).
9.3.1.3 Notched-Wedge Joints
The notched-wedge joint technique (see Figure 133) was originally designed to provide traffic a safer transition when changing lanes between the newly paved surface and the lower, existing surface. Many overlay specifications do not allow a pavement edge drop-off to remain exposed to traffic and require adjacent lanes to be completed by the end of the day. This safety feature increases production by allowing paving to continue the entire paving shift in one lane, instead of moving back at mid-shift and switching traffic control to pave an adjacent lane.

Source: Asphalt Institute
Figure 133. Notched-Wedge Joint with Taper at Top and Bottom of Wedge
The initial pass has a tapered face up to 1 ft (300 mm) in width, with a slope ranging from 3:1 to 12:1. The wedge configuration should include a notch at the top and a notch at the bottom. Notched depths of at least one NMAS are recommended.
Agencies that have adopted the use of the notched wedge generally note an increase in joint density and an improvement in the long-term performance of their LJs when compared to the butt joint. This is not the case when compared to the cutback joint. The notched wedge provides lateral support for the unconfined edge under compaction while increasing the bonding surface area between the two mats.
It is important to provide some type of compactive effort to the wedge material. Figure 134 shows a device that forms the wedge and provides some initial compaction through extrusion and vibration from the screed.

Source: Asphalt Institute
Figure 134. Notched-Wedge Device that Forms and Compacts through Screed Vibration
In Figure 135, a tow-behind wheel compactor and a tow-behind, self-vibrating plate compactor are shown.

Source: Asphalt Institute
Figure 135. Two Devices for Compacting the Wedge of a Notched-Wedge Joint
9.3.1.4 Milled or Cutback Joint
A milled or cutback joint (referred to as the cutback method) is created by physically removing 2 to 6 inches of material at the unconfined edge of the recently laid mat with either a cutting wheel (also known as a pizza cutter) or a milling machine. The cutback method offers two advantages to the LJ: providing a near-vertical edge to compact against and eliminating the area of low-density material at the unconfined edge of the first mat (see Figure 136).

Source: Asphalt Institute
Figure 136. Key Aspects to Constructing a Durable Longitudinal Joint
Both the FAA and DoD airfield paving specifications require cutting back the joint with a cutting wheel. While the cutting wheel is not common on roadway projects due to traffic control challenges and slowing production, milling back the joint is routine in Michigan for DOT work where the contractor is compensated for over-paving the joint by up to 2 inches (measured from the top of the mat).
The following standard practices should be followed when cutting back the LJ with a cutting wheel:
- The amount of material that should be cut back is generally determined by the specification. The DoD airfield specification currently says to cut back between 3 and 6 inches, while the FAA specification currently says a maximum of 3 inches.
- The cutting wheel is typically about 10 inches in diameter, with the cutting angle being about 10 to 20 degrees from vertical.
- The mix is cut back while it is still warm (120 to 140 °F) to provide the cleanest cut. This is known as the temperature sweet spot.
- The cutting wheel can be mounted on a steel-wheel roller (see Figure 137 and Figure 140) or on the blade or rear ripper of a motor grader (see Figure 138). Mounting on a short-wheelbase vehicle such as a skid steer should be avoided. If mounted on a roller, the cutting wheel can be operated on the newly paved surface. If mounted on a grader, the cutting wheel can be operated on the adjacent lane to be paved to avoid rutting on the newly paved mat that has not fully cooled.
- The trimmings should be carefully and completely removed prior to placing the hot lane. A kickout plate that pushes the trimmings away from the joint can help (see Figure 139). Any loose material must be removed, by hand if necessary. All the trimmings can be collected and used as RAP.
- It is critical that the cuts are straight and without wander to facilitate a consistent overlap on the cold mat when the hot mat is placed. Using a stringline for reference, skip paint, and a guide mounted on the front of the roller or grader for the operator to follow can help ensure a straight cut (see Figure 137, Figure 138, and Figure 140).
- No water and especially no release agent should be used to assist cutting, as this will deter the necessary bonding of the two mats.
- The cut should provide a clean, sound, near-vertical face for the full depth of lift.

Source: U.S. Army Corps of Engineers
Figure 137. Cutting Wheel Mounted on a Roller

Source: U.S. Army Corps of Engineers
Figure 138. Cutting Wheel Attached to Rear Ripper of a Grader

Source: U.S. Army Corps of Engineers
Figure 139. Kick-Out Plate Aids in Removing the Cutback Mix

Source: U.S. Army Corps of Engineers
Figure 140. Stringline, Paint, and a Mounted Guide Allow Straight Cutting
9.3.2 Rolling the Unconfined Side
Attention is key when rolling the unconfined joint because density across the mat is typically lowest at the unsupported edge. The unconfined edge should be compacted with a steel-drum roller as soon as possible while the mat is hottest.
Attention is key when rolling the unconfined joint because density across the mat is typically lowest at the unsupported edge. The unconfined edge should be compacted with a steel-drum roller as soon as possible while the mat is hottest.
There are two recommended options for a rolling pattern of the unconfined joint to optimize density. Option 1 is to roll the first pass with the steel drum overhanging the mat edge 4 to 6 inches (100 to 150 mm). More than a 6-inch overlap can cause too much force at the mat edge, resulting in excessive rolldown. Targeting less than a 4-inch overlap may result in the drum occasionally cutting into the edge of the unconfined joint. Option 2 is for the first pass to stay inside the mat edge 4 to 6 inches and the second pass overhanging the edge 4 to 6 inches. Both options are illustrated in Figure 141.
Proponents of option 2 believe there is less lateral movement of the unsupported edge under the mat. A concern with option 2 is that a stress crack can be induced at the edge of the steel drum during its first pass (4 to 6 inches inside the LJ). Such a potential stress crack may not be visible until months or years later. Proponents of option 1 are concerned with the potential for this stress crack and/or believe it is best to roll the edge when hottest.

Source: Asphalt Institute
Figure 141. Two Options for Compacting the Unconfined LJ
The following are factors to consider in deciding between option 1 and option 2:
- Density measurements close to the unsupported edge.
- Mix properties or other elements that may create excessive lateral movement.
- Excessive rolldown at the mat edge.
- Potential for stress cracks with option 2.
9.3.3 Placing the Confined Side
The following are three key considerations that should be understood when placing the hot side of the LJ that will be covered in this section:
- Tacking/bonding the near-vertical face prior to placement.
- Having sufficient rolldown mix to avoid rollers bridging on the cold mat.
- Achieving the proper overlap of the hot mat over the cold mat.
9.3.3.1 Tacking the Vertical Face
Before placing the hot lane, the cold near-vertical joint face should receive at minimum a heavy application of emulsified tack coat material, no matter whether it is a butt or cutback joint. Even a notched-wedge joint will benefit from being tacked as long as the material does not bleed up into the surface.
A more substantial treatment of the cold joint face is the application of an asphalt binder, or better yet, a rubberized joint sealant (also called joint adhesive), as seen in Figure 142. Spraying hot asphalt binder on the joint face results in more residual asphalt relative to an asphalt emulsion. The use of a rubberized joint adhesive provides the best bond at the cold joint. Many States require either the vertical face be painted with an asphalt binder or a rubberized joint adhesive be applied to improve the durability of the joint.

Source: National Asphalt Pavement Association
Figure 142. Joint Adhesive Being Applied to the Cold Joint Face
9.3.3.2 Sufficient Material for Rolldown
Figure 144 shows one of the key aspects to constructing a durable LJ is having sufficient material for rolldown. Material rolldown was discussed in Section 7.5, with the general rule of thumb being 25 percent but varying depending on the mix. The height of the uncompacted hot mat is established based on the rolldown factor. It is critical that there is sufficient thickness on the hot side of the joint for complete rolldown and compaction before the steel-wheel roller compacts down to the cold mat. If insufficient material is placed, “bridging” of the steel roller on the cold mat will occur before complete densification on the hot side is achieved. This creates a joint doomed to failure with the low-density material on the hot side of the joint, resulting in an area permeable to water and air with poor durability. A joint completed with insufficient mix thickness may initially look better but will perform worse than a well-compacted joint.
It is critical that there is sufficient thickness on the hot side of the joint for complete rolldown and compaction before the steel-wheel roller compacts down to the cold mat.
Projects with ride or smoothness specifications will require the use of mobile reference beams or skis (see Section 7.4.2.1) on the lower lifts. If the smoothness specification is met in the last intermediate lift before the surface is applied, then the surface can be paved at the required thickness with a matching grade sensor. If the surface layer requires the use of a ski to meet the final smoothness specification, the ski should only be used on the cold side of the joint and a matching grade sensor used on the hot side of the joint. Using the ski on the hot side of the joint will result in a nonuniform thickness across the joint, which can lead to lower density along the joint. This is because the ski averages the mat thickness required over the length of the ski (30 to 40 ft) and may not always provide the correct amount of mixture for the joint.
Using the grade sensor on the paver as a joint matcher device that takes a single reading just in front of the augers does a better job of getting the correct height of material at the joint. The joint matcher measures the mat thickness continuously along the joint and provides the required amount of material at each precise location. Section 7.4.2.2 covers joint-matching devices.
9.3.3.3 Proper Overlap
The other key aspect to constructing a durable LJ is to consistently maintain the correct amount of overlap from the hot mat onto the cold mat (illustrated in Figure 143). The correct amount of overlap is 1±1/2 inch (25±12.5 mm) for a butt joint. If the joint is cut back, the correct amount of overlap is less, targeting 1/2±1/2 inch (12.5±12.5 mm). As mentioned earlier, this correct overlap will be difficult to maintain if the first pass was not paved straight (or smooth for a curve). The screed operator should closely follow the joint line and monitor the overlap closely to maintain this tight tolerance. A variable-width screed (if equipped) can be helpful to move the screed in or out as necessary.
Not everyone may agree the correct amount of overlap is as recommended above, but there is no debate that some overlap is needed. Without targeting some overlap, there will be instances where there will be a gap at the joint, resulting in low density and a likely crack.
Luting (bumping) the overlap material off the cold mat and onto the hot mat is not necessary if the proper overlap (as prescribed in the above paragraph) is maintained. The small amount of overlap will not create much loose material at the surface after rolling, and that material will quickly ravel away.

Source: Frank Colella
Figure 143. Proper Overlap When Placing the Confined Side of a Longitudinal Joint
If bumping of the overlap material is done, it is crucial that the overlap material only be bumped just across onto the hot mat and not pushed farther. The rolldown material just on the hot side of the joint should not be disturbed; it must remain to achieve proper density. Aggressive luting that extends across the hot joint must be avoided as it will remove the rolldown material just on the hot side of the joint, resulting in low density as described earlier in this section. This can also cause segregated material on the surface. Improper luting of the LJ is shown in the left picture of Figure 144, while proper luting is shown in the right picture.
Aggressive luting that extends across the hot joint must be avoided as it will remove the rolldown material just on the hot side of the joint, resulting in low density.
If done carefully and correctly, luting the overlap can be beneficial. If done incorrectly, luting the overlap can cause severe joint failure.

Source: Asphalt Institute
Figure 144. Improper Luting of the LJ (left), which Starves the Hot Side of Rolldown Material,
and Proper Luting of the LJ (right)
Another consideration of whether to lute or not is safety. On roadway projects, traffic in adjacent lanes can make the luting operation very dangerous. This is not a concern for airfield projects where the entire area is closed to traffic.
Broadcasting extra material onto the hot lane should be avoided as it will result in coarse aggregate on the surface that can pop out over time, especially on airfields where FOD is a major concern. Improper broadcasting and improper luting across the joint is shown in Figure 145.

Source: Asphalt Institute
Figure 145. Improper Broadcasting and Luting across the LJ
9.3.4 Rolling the Confined Side
The confined joint should be compacted with the first pass of a steel-drum roller on the hot mat, with the edge of the drum about 6 to 12 inches (150 to 300 mm) off the LJ. The second pass is then applied by overlapping onto the cold mat by 3 to 6 inches (75 to 150 mm). The first pass creates an uncompacted strip 6 to 12 inches wide where any lateral movement pushes extra mix into this strip. The second pass then compacts this uncompacted strip with the full weight of the roller.
The primary reason for staying off the joint on the first pass is to avoid bridging the roller drum on the cold edge. As described previously in Section 9.3.3.2, “bridging” results in no further compactive effort being applied. Staying off the joint 6 to 12 inches slightly migrates the mix laterally into the joint, which results in a little extra mix and higher density in this area. This recommended rolling pattern for compacting confined joints also ensures the first and second passes occur with most of the roller on the hot mat.
Rubber tire rollers, especially vibratory rubber tire rollers, have proven to be very effective in optimizing density at the confined side of the joint.
9.4 Echelon Paving and Rolling
Watch Video
Because LJs are often susceptible to early deterioration, it is wise to reduce the number of LJs on a project where possible. If project staging and traffic control allow paving multiple lanes or shoulders in a single pass with screed extensions, at least one joint can be eliminated. Section 7.3 covered screeds and screed extensions, including photos.
Another excellent option to reduce the number of LJs is to utilize echelon paving if project staging, logistics, and traffic control allow. In echelon paving, adjacent lanes are placed and compacted side by side at the same time with multiple paving trains. The LJ created between these paving trains is called a hot joint because both sides are hot when placed and compacted. Experience has found that hot joints from echelon paving have better long-term performance compared to cold joints.
Experience has found that hot joints from echelon paving have better long-term performance compared to cold joints.
Echelon paving is not common on roadway projects because there is typically a need to maintain traffic flow, so closing multiple lanes is difficult. Airfields, large commercial parking lots, and new highway construction are examples where echelon paving should be considered (see Figure 146).

Source: Dallas Fort Worth International Airport
Figure 146. Echelon Paving with Four Paving Trains on a Runway at DFW Airport
The limiting factor on the number of paving trains utilized with echelon paving is often the overall mix production to feed the pavers. Utilizing two paving trains is the most common occurrence with echelon paving, while utilizing four paving trains, as seen in Figure 146, is extremely rare.
Lanes are placed simultaneously with the pavers separated by only a short distance, usually less than 100 ft (30 m). This short distance allows the mats to effectively be welded together by the compaction train before the mix on either side of the joint cools. Overlap is typically targeted at 1 inch (25 mm).
Having a standard rolling train behind each paver is recommended. To maximize density at the hot joint, the breakdown roller following the lead paver should leave approximately 4 to 6 inches (100 to 150 mm) of the common edge or joint unrolled. This common joint is then compacted by the first pass of the breakdown roller following the second paver. To accomplish this effectively, the second paver must keep as close as possible to the first paver to minimize any temperature difference between each side of the joint. The material on each side becomes a single mass under the roller, and there is little or no difference in density between the two lanes.
9.5 Unconventional Longitudinal Joint Methods
This chapter has already discussed many LJ techniques, options, and products that may not be considered “conventional.” They include the following:
- Always having confinement when placing and rolling the LJ (Sections 9.3.3 and 9.3.4). This can be achieved by milling and then paving one lane at a time versus milling multiple lanes.
- Paving wider and echelon paving (Section 9.4).
- Milling or cutting back the joint (Section 9.3.1.4).
- Rubberized joint adhesives applied to the face of the joint (Section 9.3.3.1).
- Utilizing rubber-tire (pneumatic) rollers when compacting the hot side of the joint (Sections 9.3.4 and 8.3.2).
There are three other unconventional techniques not yet mentioned: joint heaters, surface sealers, and void-reducing asphalt membrane (VRAM). All three were developed with the intent of improving LJ performance. They are not being endorsed by the authors or sponsors of this Handbook but rather are mentioned to be inclusive of other unconventional techniques not already mentioned here.
Joint heaters—The use of infrared joint heaters to heat the face of the cold joint just prior to placing the confined side. These heaters are used most frequently in cold climates and cold-weather paving. Some recent studies have shown heaters can improve joint density by 1 to 2 percent. Care must be taken to not overheat the joint and cause damage to the binder. Heater technology has improved to include longer and more efficient infrared heaters and automation with paver speed to minimize overheating or underheating the joint. Figure 147 shows the two general types of joint heaters: those that are self-contained units operating in front of the paver and those mounted on the paver itself.

Source: Asphalt Institute
Figure 147. Joint Heaters: Self-Contained (left) and Paver-Mounted (right)
Surface sealer and rejuvenator products—These are sprayed on top of the completed joint with a typical width of 1 to 2 ft. These topical treatments are applied either when the joint is new or after the joint has been in service for some time. Some States use them as a remedial action for not meeting a minimum density at the joint. These products seal the joint from the top down to reduce absorption and permeability. They are also referred to as a joint stabilizer or joint enrichment. Another type of joint sealer product is called rapid penetrating emulsion (RPE), which is an asphalt emulsion containing about 30 to 40 percent asphalt binder designed to penetrate voids in the asphalt pavement. The penetrating nature of the RPE is important because it carries the asphalt residue into the voids and reduces air and water intrusion while maintaining pavement texture. Figure 148 shows an application of RPE and an application of a rejuvenator that dries clear. Restriping is necessary with RPE and other asphalt-based surface sealers such as fog seals or microsurfacing, but it is not necessary with many of the rejuvenator products that dry clear. These surface sealers are often used over centerline rumble strips. Like all these unconventional techniques, more research is needed on long-term benefits.

Source: Asphalt Materials, Inc.
Figure 148. Surface Sealers on LJs: RPE (left) and Rejuvenator VRAM (right)
Rather than sealing the LJs from the top down, the product called VRAM is designed to seal the LJ from the bottom up. Use of VRAM involves applying a heavy band (1 gal/yd2 for a 1.5-inch overlay) about 18 inches wide of polymer-modified asphalt binder to the area where the new joint will be centered. The cold side is placed and compacted, passing over half the width of the band. Figure 149 shows two methods of placing the thick band and then paving over it. The hot side is placed and compacted as a conventional joint. The polymer-modified binder migrates into the mix at the joint, filling voids from the bottom up, reducing water intrusion at the joint and protecting underlying pavement layers. There currently is no proven way to get an exact measurement of in-place air voids of mixes where VRAM is used.

Source: Asphalt Materials, Inc.
Figure 149. VRAM Is Applied with Manual Strike-Off Box (left) or Modified Distributor (middle), then Paved Over (right)