11. Quality Assurance
11.7 Quality Control In The Field: Placement And Compaction
QC tests and measurements should take place throughout the day during placement and compaction. The success of QC during placement depends on making corrections while the mix is hot and when a problem can be actively corrected.
11.7.1 Temperature Requirements
Because asphalt binder is a thermoplastic material, its properties change considerably with changes in temperature. Asphalt mixture is most workable and compactible when the material is hot. Most specifications have temperature requirements in several key areas.
11.7.1.1 Maximum Mixture Temperature
The asphalt mixture’s maximum temperature is often specified to avoid premature aging and oxidation of the mix. A typical maximum limit is 325 °F (163 °C). Sometimes the maximum limit is extended to 350 °F (177 °C) for polymer-modified mixtures. Of course, the limit is lowered when producing WMA to be used at cooler temperatures. The actual limit may be different for different WMA technologies. Contractors often use WMA technology as a compaction aid at HMA temperatures. This practice should not be discouraged because of the great importance of proper mat compaction.
The maximum temperature is best verified in a location close to where the mix is discharged, as soon as possible after mixing. A great location for drum-mix plants is the discharge chute from the drum to the slat conveyor, as shown in Figure 164. Infrared thermometers are the best tool for measuring temperature in this location.

Source: Asphalt Institute
Figure 164. Mix Being Discharged from the Drum
11.7.1.2 Minimum Temperature Immediately Behind the Screed
The loose mat’s minimum temperature immediately behind the screed is often specified to facilitate compaction. If a mat is too cool before the rollers hit it, it will be impossible to achieve proper mat density. A typical minimum limit is 250 °F (121 °C). It should be clearly understood that this temperature is a minimum, not a target. Again, the limit is often lowered when placing WMA.
The measuring location should be as close as possible to the back of the screed. Again, infrared thermometers are a great tool as long as a roller has not yet reached the measurement location. Roller drums are typically sprayed with a soapy water solution to keep the mix from sticking to the drum. This solution can lower the temperature of the extreme top surface of the mat and result in erroneous information from an infrared gun. If a roller has already made a pass over the measurement location, a stab thermometer will give the best results for the true mat temperature.
11.7.1.3 Minimum Ambient or Surface Temperature
An asphalt mixture will retain heat well while it is in the back of a truck. As discussed in Section 8.4.2, the heat dissipates rapidly once it is placed, especially with thinner lifts. This is one reason why paver operators should not speed up if several trucks are lined up in front of the paver, leaving roller operators behind. If the existing surface is already cool, the heat in the mix will dissipate even more rapidly. Most specifications have a minimum ambient temperature or a minimum surface temperature to facilitate the mat’s heat retention. Thicker mats retain heat better than thinner mats, so there is often a mat thickness component to the specification as well. Allowances may also be made for WMA versus HMA. As an example, Table 12 shows base temperature requirements from the FAA’s P-401 specification for airport construction.
Table 12. FAA Surface Temperature Specification

Source: FAA advisory circular 150/5370-10H (Table 4 of Item P-401)
11.7.1.4 Minimum Surface Temperature for Finish Rolling
An asphalt mat will remain compactible until the binder temperature becomes so low that aggregate in the mat begins to break under the finish roller. To protect the mat, many agencies specify a minimum surface temperature for finish rolling, often around 140 °F (60 °C). Because the job of the finish roller is to iron out any marks and achieve final smoothness, mat density should have already been achieved well before the mat temperature drops to this level.
11.7.2 Test Strips
Watch Video
Test strips, or “control strips,” are often constructed before beginning regular production paving for each asphalt mixture. Just as a trial batch ensures that the plant can produce a mix that meets specifications, a test strip ensures that the field crew can place and compact a mat that meets specifications. They also allow a second opportunity to verify the mix and the agreement of test results between labs. Test strips are composed of shorter lengths of pavement, typically 500–1,000 ft (150–300 m). The FAA control strip requirements for airfields are based on either tonnage (minimum 250) or 1/2 sublot, whichever is greater. FAA and DoD airfield test strips are also required to include two paving lanes with a longitudinal cold joint between them.
Just as a trial batch ensures that the plant can produce a mix that meets specifications, a test strip ensures that the field crew can place and compact a mat that meets specifications.
If possible, the test strips should be constructed on the project, with the same equipment and materials that will be used for the rest of the project. Some circumstances may warrant the test strip being placed in another location.
If the results of the test strip indicate the JMF is suitable for producing complying materials, and the appropriate spreading, placing, and compaction can be achieved, then production paving can proceed. If the results of the test strip do not meet project specifications, or if the typical existing cross-section changes, then adjustments can be made and a new test strip produced.
The following listing of placement controls should be closely monitored by the contractor:
- Tack coat application.
- Asphalt mix delivery rate.
- Paver speed.
- Paver adjustments.
- Grade control.
- Thickness control.
- Density control—
- Temperature of air and mixture.
- Roller type.
- Rolling pattern and coverage.
- Roller speed.
- Yield thickness control.
- Smoothness control.
11.7.3 Mat Density
Watch Video
The goal of compacting an asphalt pavement is to achieve proper density. The resulting in-place air void content of the asphalt mat is, in many ways, the single most important factor that affects the performance of the mixture throughout the life of the pavement.
The goal of compacting an asphalt pavement is to achieve proper density. The resulting in-place air void content of the asphalt mat is, in many ways, the single most important factor that affects the performance of the mixture throughout the life of the pavement.
Compaction is affected by many factors other than those specifically measured during placement of the mixture. This means that low density problems on a project may not be resolved simply by adjusting the rolling pattern or the temperatures. The QC manager and project superintendent may need to analyze all the QC data, including that from the mixture production, to address compaction problems.
In addressing a compaction problem, the paving crew must review their own operations and procedures for the placement and compaction operation, paying particular attention to temperatures and to having a disciplined adherence to good rolling technique and consistent and tested rolling patterns.
A variety of methods are available to control the quality of the compaction for an asphalt mixture. Those methods will be discussed in more detail below. These methods are usually driven by specification, however, so the QC will be based on the specified methods for acceptance of compaction. The QC efforts should be centered on establishing and documenting compliance with the actual specifications.
There are three ways to calculate compaction values, and they each give very different results. Compaction can be specified by the percentage of the TMD, the bulk laboratory density, or a control strip density. It is best practice, and most commonly specified, to measure density as a percentage of the TMD. For airfields, the FAA and DoD formerly specified density as a percentage of laboratory density, but the current P-401 and UFGS 32 12 13.15 specifications have moved to a percentage of theoretical maximum. The method specified should be clearly understood by both the agency and the contractor.
A common control method for compaction is to simply measure the in-place density. These measured densities will be compared with the specified reference density (typically TMD), and a percentage of the reference density will be calculated. Nuclear density measurements are the most common form of QC density testing for quick feedback to guide roller patterns. Non-nuclear devices have been developed and are gaining popularity for QC density testing. QC testing for density can also be done using cores; however, this imparts a delay in the results. Use cores to correlate and/or calibrate other test methods, especially if gauge readings are to be used for acceptance. Many agencies and gauge manufacturers have devised methods to properly correlate gauge readings to core results.
11.7.4 Mat Smoothness
Watch Video
Mat smoothness for QC and acceptance purposes is measured after compaction, typically with either a 10-ft straightedge (FAA and DoD specify 12-ft), a profilograph, or an inertial profiler.
Spot checks are typically done with the straightedge laid on the pavement and the deviation of the surface measured and recorded. Typically, no bumps or dips greater than 1/8 inch are allowed when measured from the two outer edges of the straightedge. Specifications usually require these measurements be taken in both the longitudinal and the transverse direction. By mounting a small set of wheels on the straightedge, spot checks can be performed immediately behind the finish roller while compaction is ongoing. This immediate feedback to the paver and the roller operators allows them to make the appropriate adjustments to correct smoothness issues before the mix cools. FAA requires that deviations greater than 1/4 inch that will trap water on the final surface in either the transverse or longitudinal direction be diamond ground and sealed.
The profilograph has historically been the method used to measure the roughness of new construction and overlay projects for acceptance. The profilograph is typically manually pushed along by the technician, requiring a lane closure for safety reasons. The use of this technology has waned in recent years as faster, more accurate inertial profilers are now preferred.
Inertial profilers can collect true pavement profile data and longitudinal distance data at highway speeds. Lightweight versions of the inertial profilers operate at slower speeds and can be used almost immediately after finish rolling to provide more timely measurements.